Potters & Sculptors - Making Rock from Mud
Ron Roy has asked me to test some fake ash glazes to see if he can develop a fake ash that does not have pinholes or any bubbles.
If any one would like to test these and get back to the group with results I would be grateful as it will probably be a few weeks before I can fire again.
Here are the glazes.
Recipe Name: Fake Ash Test 1
Cone: 6 Color: Ash
Firing: Oxidation Surface: Glossy
Amount Ingredient
47 Red Art
22 Whiting
13 Nepheline Syenite
4 Frit--Ferro 3134
14 Dolomite
100 Total
Recipe Name: Fake Ash Test 2
Cone: 6 Color: Ash
Firing: Oxidation Surface: Glossy
Amount Ingredient
46.5 Red Art
22 Whiting
13 Nepheline Syenite
5.8 Frit--Ferro 3134
12.8 Dolomite
100 Total
Recipe Name: Fake Ash Test 3
Cone: 6 Color: Ash
Firing: Oxidation Surface: Glossy
Amount Ingredient
46 Red Art
22 Whiting
13 Nepheline Syenite
7.5 Frit--Ferro 3134
11.5 Dolomite
100 Total
Recipe Name: Fake Ash Test 4
Cone: 6 Color: Ash
Firing: Oxidation Surface: Glossy
Amount Ingredient
45.5 Red Art
22 Whiting
13 Nepheline Syenite
9.3 Frit--Ferro 3134
10.3 Dolomite
100 Total
Recipe Name: Fake Ash Test 5
Cone: 6 Color: ash
Firing: Oxidation Surface: Glossy
Amount Ingredient
45 Red Art
22 Whiting
13 Nepheline Syenite
11 Frit--Ferro 3134
9 Dolomite
100 Total
Tags:
I like this. I know I'm coming late to the party, but are these as green as they appear on my monitor? (olive clear color) and on the sushi plate and vase, did you also brush the pseudo ash on?
Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase
Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com
Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.com. Mastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.
Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.
The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.
Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .
If you are up to creating videos of your work or techniques you might want to invest in a flip video camera
Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00
And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62
ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.
If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014
Switch to the Mobile Optimized View
© 2026 Created by Andrea Wolf.
Powered by