Has anyone come close to the look of Alisa Clausen's ^6 "Cassie's Marsala" where she uses MOK-623 frit?

56.6 Red Art Clay
20.0 Frit 169/MOK 623
9.4  Nepheline Syenite
9.4  Talc
5.7  Bone Ash
6.6  Iron Oxide-Red

Using the analysis for the Johnson Matthey Frit 623 I made a chemically similar glaze, but it's missing the glassy look produced by a pre-melted frit.

http://digitalfire.com/4sight/material/johnson_matthey_frit_623_647...

The Original   http://www.flickr.com/photos/glazes/1084681129/

Three glazes I've made with Alisa's recipe, replacing the MOK-623 frit with substitutions to match the chemical makeup. Of course I have tiles from other versions which are too ugly to merit posting.

#1.)  Cassie's Marsala using substitutions for MOK-632 and Red Iron Oxide Precipitate from Standard Ceramics

#2.)  Cassie's Marsala using Ferro Frit 3249 instead of MOK-632 frit and Red Iron Oxide from Laguna Clay / Axner.

#3.)  Cassie's Marsala using Laguna Clay / Axner Red Iron Oxide and 25% additional 3134 Ferro Frit to create a similar glassy look.

Views: 915

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Norm Stuart on March 14, 2013 at 4:44pm

This is the mix I've used as a replacement for MOK-623.

 

MOK-623 Replacement

75.0%    Ferro Frit 3134
30.0%    Borax
10.0%    Soda Ash
  5.8%    Zinc Oxide
  5.3%    Strontium Carbonate
(12.8%)  Calcium Oxide

 

This particular mix provides 12.8% too much Calcium Oxide, resulting in 2.5% too much Calcium Oxide in the final glaze, which could make the glaze a little too much like a Calcium Semi-matte.

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2025   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service