Title says it all.I find what the Obsidian over the SCM does to be interesting.

Views: 289

Comment

You need to be a member of Electric Mid&Hi Fired Ceramics to add comments!

Join Electric Mid&Hi Fired Ceramics

Comment by Jeff Poulter on May 23, 2014 at 9:24am

So I mixed up some Obsidian last night.  I was worried about  cracking and crawling with the Alberta Slip at such a high percentage of the glaze, so I did 40 Alberta Slip & 35 Ohio Slip.  Even when layered, there were no cracking issues at all.  The kiln is cooling as we speak, so I might have pics to post when I get home, unless they are butt-ugly!  jhp

Comment by Jeff Poulter on May 22, 2014 at 11:17am

Eric Preece had a ^6 version of Obsidian that he used.  Off of his website, it is:

Alberta Slip   75

FF 3134    25

Cobalt Carb   5

     I can't remember if I tried it or not.  I may have to whip some up using Alberta slip & maybe try some using Ohio slip as well.  Could even use some Ravenscrag, but would have to throw some RIO in to make it comparable.  So little time, so much to test!!!!  jhp

Comment by Joe Shaw on May 21, 2014 at 9:38pm
The recipe for Obsidian is from Richard Aerni.

Alberta Slip 91.0
Cobalt Ox. 9.0

Instead ofCobalt Oxide I use Robin Hopper's Black Stain.

Black Stain (Robin Hopper)

Cone: Color: Black
Firing: Ox. or Red. Surface:

Amount Ingredient
20 Iron Oxide--Black
20 Manganese Dioxide
20 Cobalt Oxide
20 Chromium Oxide
8 Kaolin--EPK
8 Feldspar--Custer
4 Silica

100 Total
Comment by George Lewter on May 21, 2014 at 1:07pm

Is the "obsidian" the commercial glaze from AMACO?

Comment by Donna Kat on May 21, 2014 at 7:39am

This is so striking.  I am surprised I missed it and only found it because I was looking for your profile picture to link to for someone asking about Steven Hill glazing.

Comment by Carl Ray Crutchfield on June 22, 2012 at 11:24am

Beautiful color variations.

Videos

  • Add Videos
  • View All

Use These Links to Support Us

Low cost flat lapping disc can be used on you potters wheel if you, drill bat pin holes in it, and provide a trickle of water to cool it. At amazon.com, 120 grit for aggressive material removal. Click the image to purchase 

Members have had great things to say about John Britt's new book, Mid-Range Glazes. Click the image to buy from Amazon.com

Purchase Glazes Cone 6 by Michael Bailey, The Potters Book of Glaze Recipes by Emmanuel Cooper, or Making Marks by Robin Hopper, all available at amazon.comMastering Cone 6 Glazes by John Hesselberth & Ron Roy is now out of print.

Harbor Freight is a great place to find unbeatable prices for better HVLP spray guns with stainless steel parts and serviceable economy models, as well as detail guns, all tested by our members for spraying glazes, as well as compressors to power the guns. As yet no one has tested and commented on the remarkably inexpensive air brushes at harbor freight.

The critter siphon gun is a spray alternative that is well liked by some of our members, and is available at amazon.

Amazon is also a competitive source for photo light tents for shooting professional quality pictures of your work. They also have the EZ Cube brand favored by several of our members. You might also want to purchase the book Photographing Arts, Crafts and Collectibles . . .

If you are up to creating videos of your work or techniques you might want to invest in a flip video camera

Following are a few scales useful for potters. Ohaus Triple Pro Mechanical Triple Beam Balance, 2610g x 0.1g, with Tare $169.00

And finally a low cost clone of the OHaus. The Adam Equipment TBB2610T Triple Beam Mechanical Balance With Tare Beam $99.62

ebay is a great alternative for many tools and the equipment used in the ceramics studio - kilns, wheels, extruders, slab rollers are often listed there both new and used.

Tips for Members

If you just want to spout off, it is best accomplished as a blog posting. If you want to get more guidance and ideas from other members, ask a question as a new discussion topic. In the upper right corner of the lists for both types of posting, you will find an "+Add " button. Clicking it will open an editor where you create your posting. 4/16/2014

© 2024   Created by Andrea Wolf.   Powered by

Badges  |  Report an Issue  |  Terms of Service