by Jan Wallace
Apr 11, 2012
Emily's Purple - Opaque Blue/Purple
Custer Feldspar (I used Potash Feld) 36.60
Gerstley Borate 19.40
Ball Clay 11.80
Talc 15.10
Silica 10.80
Dolomite 6.50
Zircopax 10.00
Cobalt ox 3.00
Total 113.20
Cool to 900c, hold for 1 hr. Lovely smooth blue/purple, opaque glaze.